Causes and solutions of top whiteness in injection molding products

Release time:2021-08-16

When the plastic parts of injection products are ejected from the mold, if the ejector pin is used, the ejector rod will often leave deep or shallow marks on the plastic parts. If these traces are too deep, the so-called top white phenomenon will appear. In serious cases, the so-called top explosion will occur when the plastic parts are pushed through.


The main reason for the whiteness of plastic parts is that the product has a large mold adhesion force, and the ejection part on the plastic parts causes white marks at the ejection part of the ejector rod. The specific reasons and improvement methods are as follows:


1. Back mold temperature is too low or too high: adjust the appropriate mold temperature.


2. Too fast ejection speed: slow down the ejection speed.


3. With demoulding chamfer: overhaul the mold (polishing).


4. The ejection of finished products is unbalanced (the ejection leaf spring is broken): repair the mold (make the ejection balanced).


5. Insufficient number of thimbles or improper position: increase the number of thimbles or change the position of thimbles.


6. Vacuum occurs in the mold during demoulding: clean the dirt in the ejector pin hole to improve the air inlet effect.


7. The finished bone and column positions are rough (inverted): polish each bone and column position.


8. High injection pressure or holding pressure: reduce the pressure appropriately.


9. The demoulding angle of the finished mold is too small: increase the demoulding angle of the rear mold.


10. Improper action time or position of side slider: repair the mold (make the core pulling action normal).


11. Ejection area is too small or ejection speed is too fast: increase the ejection area or slow down the ejection speed.


12. The injection speed of the last section is too fast (Burr): slow down the injection speed of the next section.


These are the reasons and solutions for the whitening of injection molded products.

Copyright: Shenzhen Zhongyuan Plastic Co., Ltd. | mold processing customized manufacturer. If you want to know the processing price of the factory, how much is it, and which is good, please contact us Yue ICP Bei No. 17060480
主站蜘蛛池模板: 三级黄网站| 撕开奶罩揉吮奶头视频| 天天综合天天添夜夜添狠狠添| 国产精品久久久午夜夜伦鲁鲁| 东北少妇不带套对白| 国产成人精品视频网站 | 涩涩高清无乱码在线观看| 中文区中文字幕免费看| 色综合色天天久久婷婷基地| 无遮挡1000部拍拍拍免费| 国内精品人妻无码久久久影院导航| 中文字幕一区二区三区精彩视频| 亚洲av无码电影在线播放| 网友偷自拍原创区| 人妻饥渴偷公乱中文字幕| 国产精品天天看大片特色视频| 国产精品亚洲一区二区三区在线 | 老头边吃奶边弄进去呻吟| 天天操夜夜爽| www夜片内射视频日韩精品成人| 久久天堂av综合色无码专区| 久久丫精品国产亚洲av| 内射老阿姨1区2区3区4区| 好黄好硬好爽好刺激| 久久99精品久久久久久hb无码| 国产高清在线精品一区不卡| 极品少妇被猛得白浆直流草莓视频| 亚洲精品无码久久一线 | 欧美阿v高清资源在线| 电源天堂| 把女邻居弄到潮喷的性经历| 欧美疯狂xxxx乱大交| 久久午夜影视| 海角国精产品一区一区三区糖心| 免费乱理伦片在线观看夜| 少妇做爰免费视频网站| 成人精品一区二区三区中文字幕| 性视频久久| 亚洲av无码一区二区三区系列| 亚洲成a∨人片在无码2023| av天堂中av世界中文在线播放|